Thermal Electrical Properties Table Chart Iron per BS2789
Engineering Materials Database
This table defined the thermal and electrical properties of ductile iron grades covered UK specification BS2789.
Grade |
Thermal conductivity,
100 °C (212 °F) |
W/m · K
(Btu/ft · °F) at 500 °C (930 °F) |
Specific heat capacity,
20-700 °C (68-1290 °F) |
Coefficient of
thermal expansion at 20-400 °C (68-750 °F), 10-6/K |
Electrical resistivity,
μΩ/m |
|
J/kg · K
|
Btu/lb · °F
|
|||||
Ferritic Grades
|
||||||
350/22;
350/22L40 |
36.5 (21.1)
|
35.8 (20.7)
|
603
|
0.144
|
12.5
|
0.500
|
400/18;
400/18L20 |
36.5 (21.1)
|
35.8 (20.7)
|
603
|
0.144
|
12.5
|
0.500
|
420/12
|
36.5 (21.1)
|
35.8 (20.7)
|
603
|
0.144
|
12.5
|
0.500
|
Intermediate Grades
|
||||||
450/10
|
36.5 (21.1)
|
35.8 (20.7)
|
603
|
0.144
|
12.5
|
0.500
|
500/7
|
36.5 (21.1)
|
34.9 (20.2)
|
603
|
0.144
|
12.5
|
0.510
|
600/3
|
32.8 (18.9)
|
32.2 (18.6)
|
603
|
0.144
|
12.5
|
0.530
|
Pearlitic as Cast and Normalized Grades
|
||||||
700/2
|
31.4 (18.2)
|
30.8 (17.8)
|
603
|
0.144
|
12.5
|
0.540
|
800/2
|
31.4 (18.2)
|
30.8 (17.8)
|
603
|
0.144
|
12.5
|
0.540
|
900/2
|
31.4 (18.2)
|
30.8 (17.8)
|
603
|
0.144
|
12.5
|
0.540
|
Hardened and Tempered Grades
|
||||||
700/2
|
33.5 (19.4)
|
32.9 (19.0)
|
603
|
0.144
|
12.5
|
0.540
|
800/2
|
33.5 (19.4)
|
32.9 (19.0)
|
603
|
0.144
|
12.5
|
0.540
|
Related:
- Steel Section Properties Chart Narrow I-Beam BS 4-1 | EN 1993-1-1
- Steel Section Properties Chart Wide I-Beam BS 4-1 | EN 1993-1-1
- Structural Steel Angle Section Properties, Unequal Leg BSI BS EN 10056
- Structural Steel Angle Section Properties, Equal Leg BSI BS EN 10056
- Structural Steel I-Beam Universal Flange Section Properties BS 4-1:2005
- Structural Steel I-Beam Universal Flange Section Properties BS4: Part 1: 1993