Related Resources: materials

Laminate Glass Cloth Engineering Properties

Engineering Materials

Wet Laminate Glass Cloth engineering properties in imperial units.

Wet Laminate Glass Cloth

Description
Hot Wet
Hot
RT
Cold
Minimum
(160F, 95% RH)
(160F)
(75F)
(-65F)
F tu1 (psi)
42815
51169
54824
59132
42815
E t11 (psi)
3698462
3698462
3698462
3698462
3698462
F tu2 (psi)
34335
39421
41901
46470
34335
E t22 (psi)
3698462
3698462
3698462
3698462
3698462
v 12
0.16
0.16
0.16
0.16
0.16
F cu1 (psi)
48191
51300
62004
71663
48191
E c11 (psi)
3698462
3698462
3698462
3698462
3698462
F cu2 (psi)
48191
37724
34069
53388
34069
E c22 (psi)
3698462
3698462
3698462
3698462
3698462
F su12 (psi)
11255
12531
15664
19188
11255
G 12 (psi)
638166
638166
638166
638166
638166
ILS
-
-
-
-
0
Thickness (in)*
0.0118
0.0118
0.0118
0.0118
-
E av11 (psi)
3698462
3698462
3698462
3698462
3698462
E av22 (psi)
3698462
3698462
3698462
3698462
3698462
CAI Compression Strain
6000.0
6387.0
7719.7
8922.4
6000.0
Filled Hole Tension Strain
8000.0
9561.0
10243.9
11048.8
8000.0
Open Hole Tension Stress (psi)
-
-
-
-
-
Open Hole Compression Stress (psi)
-
-
-
-
-
Filled Hole Tensions Stress (psi)
-
-
-
-
-
Filled Hole Compression Stress (psi)
-
-
-
-
-
50% Bypass Tension Stress (psi)
-
-
-
-
-
50% Bypass Compression Stress (psi)
-
-
-
-
-
25% Bypass Tension Stress (psi)
-
-
-
-
-
25% Bypass Compression Stress (psi)
-
-
-
-
-
Single Shear Bearing Stress (psi)
-
-
-
-
-
Double Shear Bearing (psi)
-
-
-
-
-
* Check Thickness Values against specific project material